Home >> General Troubleshooting of Plastic Molding
Silver Mark, Air Bubble, Production not Glossy
Trouble Shooting for Product Defects

silver mark, air bubbleProduction not glossy
reason solution reason solution 
  machine Nozzle temperature is too high lower temperature Raw material  is not enough increase injecting pressure, speed and raw material 
injecting speed too fast Reduce speed 
injecting pressure too high Reduce pressure 
mould mould temperature too low increase mould temperature mould temperature too low increase mould temperature 
Melting plastic flow improperly in the mould change injecting sprue location, adjust mould temperature, make plastic part thickness  average Mould release is too much clear 
Mould cavity is dirtcheck and clear 
material Too much moisture in material dry material, increase back pressure 

temperature too high Reduce temperature 
material dirt change material 
material not fully mixed fully mixed material 
Mixed grain is not uniformchange to uniform plastic 
not lubricate enough add lubrication such as 0.03% NINC STEARATE