Trouble Shooting for Product Defects |
| Black spots | black mark |
reason | solution | reason | solution |
machine | Plastic is heated in barrel, temperature is too high,or time is too long | Empty plastic and clean barrel, reduce barrel temperature and heating time | The screw rotation speed is too fast, or barrel & screw is not concentric | reduce screw speed, adjust the concentricity of barrel & screw |
Production has Burning mark when inject into mould | Reduce injection pressure speed | Nozzle hole is too small or temperature is too high | enlarge hole or reduce nozzle temperature |
There have die corner, make plastic overheat in barrel | Check up area of nozzle and barrel, find and remove gaps or corrosion |
|
|
|
|
mould | Burn mark | Add mould venting groove,change the gate |
|
|
material | foreign objects in plastic | check up material, empty plastic in the barrel | Barrel temperature is too high | reduce barrel temperature |
Burn mark | reduce the material temperature |